PA6 BKV 30 H2.0 EF 901510µÂ¹úÀÊÊ¢Durethan 30%²£ÏËÔöÇ¿ÄÍÈÈÀÏ»¯Îȶ¨ÄáÁú6ËÜÁÏ£¨18024445500£©
PA 6, 30 % glass fibers, injection molding, improved flowability, heat-aging stabilized
ISO/ ASTM
ISO Shortname: ISO1874-PA 6, GHR, 10-090, GF30
Property Test Condition Unit Standard guide value
d.a.m. cond.
Rheological properties
C Molding shrinkage, parallel 60x60x2; 280 ¡ãC / MT 80 ¡ãC; 600 bar % ISO 294-4 0.29¡¡
C Molding shrinkage, transverse 60x60x2; 280 ¡ãC / MT 80 ¡ãC; 600 bar % ISO 294-4 0.81¡¡
Post- shrinkage, parallel 60x60x2; 120 ¡ãC; 4 h % ISO 294-4 0.05¡¡
Post- shrinkage, transverse 60x60x2; 120 ¡ãC; 4 h % ISO 294-4 0.1¡¡
Mechanical properties (23 ¡ãC/50 % r. h.)
C Tensile modulus 1 mm/min MPa ISO 527-1,-2 9400 5500
C Tensile Stress at break 5 mm/min MPa ISO 527-1,-2 170 100
C Tensile Strain at break 5 mm/min % ISO 527-1,-2 3.0 5.8
C Charpy impact strength 23 ¡ãC kJ/m² ISO 179-1eU 65 80
C Charpy impact strength -30 ¡ãC kJ/m² ISO 179-1eU 55 55
C Charpy notched impact strength 23 ¡ãC kJ/m² ISO 179-1eA 11 15
C Charpy notched impact strength -30 ¡ãC kJ/m&sup2; ISO 179-1eA <10¡¡
Izod impact strength 23 ¡ãC kJ/m&sup2; ISO 180-1U 60 75
Izod impact strength -30 ¡ãC kJ/m&sup2; ISO 180-1U 55 50
Izod notched impact strength 23 ¡ãC kJ/m&sup2; ISO 180-1A 10 20
Izod notched impact strength -30 ¡ãC kJ/m&sup2; ISO 180-1A <10¡¡
Flexural modulus 2 mm/min MPa ISO 178-A 8400 5000
Flexural strength 2 mm/min MPa ISO 178-A 260 170
Flexural strain at flexural strength 2 mm/min % ISO 178-A 3.6 5.5
Flexural stress at 3.5 % strain 2 mm/min MPa ISO 178-A 255 140
C Puncture maximum force 23 ¡ãC N ISO 6603-2 803¡¡
C Puncture maximum force -30 ¡ãC N ISO 6603-2 744¡¡
C Puncture energy 23 ¡ãC J ISO 6603-2 2.2¡¡
C Puncture energy -30 ¡ãC J ISO 6603-2 2.1¡¡
Ball indentation hardness¡¡N/mm&sup2; ISO 2039-1 193 |